The Little Bump Does All The Work: How Fasteners Are Welded On

2026/11/23

últimas notícias da empresa sobre The Little Bump Does All the Work: How Fasteners Are Welded On

The Little Bump Does All the Work: How Fasteners Are Welded On

A nut welded to a steel sheet is not welded around its circumference. It is welded at three or four small bumps stamped into its flange, and those bumps are consumed in the process: they collapse, the nut settles onto the sheet, and a nugget forms where each bump used to be.

The process is called projection welding, and almost everything that goes wrong with welded fasteners comes from forgetting that the projection is the electrode. It is the only part of the assembly that concentrates current, and it exists for a few milliseconds.

últimas notícias da empresa sobre The Little Bump Does All the Work: How Fasteners Are Welded On  0

Truck sill beams stacked at a customer's plant, each with round weld nuts fixed along the top face. Every one of those nuts is held by three or four small projections that no longer exist.

Why a Bump Welds and a Flat Face Does Not

Current takes the path of least resistance, and between two flat surfaces pressed together that path is everywhere at once. A flat nut on a flat sheet would carry the current across the whole flange area, which means the current density is low everywhere, which means nothing reaches melting point before the heat is conducted away into the sheet and the platen.

A projection changes the geometry of that contact. Three small bumps mean the current is forced through three small areas, the density rises by one or two orders of magnitude, and the metal at the tip of each bump reaches melting temperature while the rest of the flange is still cold. The bump also increases the local resistance, which is the same thing said in the language of the electrical circuit.

Then the bump collapses under the electrode force. The nut drops by the height of the projection — a few tenths of a millimetre — and the molten metal at each tip is forged into the sheet. The force is held for a moment after the current stops, which is what turns a fused contact into a joint that survives torque.

The Conditions That Have to Be True

Four conditions have to hold at the same instant, and each of them is a production variable rather than a design variable. The projections have to be the highest point of the assembly, so that they touch first. They have to be the same height as each other, so that all three or four carry current. The sheet underneath has to be supported flat. And the electrode has to sit on the nut squarely, because a tilted electrode loads one projection harder and starves the others.

A burr from the punching operation breaks the first condition. The nut rides on the burr, one projection never contacts, the remaining three take all the current and collapse too fast, and the joint that results is held by two or three spots instead of four. It will pass a visual check and it may pass a torque test, and it will come apart on the line where the part is actually used.

A worn stamping die breaks the second condition. Projection height is formed by the die, and after a regrind or a long run the height drops by a few hundredths of a millimetre. That is enough to change how the load divides between the projections, and it is invisible on the finished part.

últimas notícias da empresa sobre The Little Bump Does All the Work: How Fasteners Are Welded On  1

The same parts from a lower angle. The nut flange sits flat on the sheet, which is the condition the whole process depends on and the one that is easiest to lose in production.

The Coating Changes the Circuit

Most weld nuts are zinc plated and most of the sheet they are welded to is galvanised, so the first thing the projection touches is not steel. Zinc melts at 419 °C and boils at 907 °C, both of them well below the melting point of the steel underneath, so the coating at the tip of the projection turns to vapour before the joint has formed. That vapour has to go somewhere, and where it goes is into the metal that is trying to become a nugget.

The practical consequences are two. The contact resistance at the start of the weld is not the resistance of steel on steel, so a schedule developed on bare sheet will not transfer to coated parts without adjustment. And the collapse happens earlier and less predictably, because the projection is sitting on a layer that gives way at a lower temperature than the metal it is supposed to fuse into.

The usual answer is more current and slightly more time, which sounds like the answer to everything and is not: on a thin sheet under a nut, more current is how the hole gets blown. The better answer is to keep the two variables that matter under control — coating mass on the sheet and plating thickness on the nut — and to prove the schedule on the coated parts rather than on a bare coupon from the same thickness.

The Platen Is a Wear Part

Under the sheet there is a flat copper or copper-alloy platen, and it does the same job as an electrode face. The projections are hot and they are small, and over a few thousand parts they leave a pattern of pits in the platen exactly where the nuts sit. A pitted platen supports the sheet unevenly, the nut leans, one projection carries more current, and the process drifts without any setting being changed.

We treat platen condition as a scheduled item rather than a fault to be found later. Face it flat on a known interval, and check it whenever a batch shows a nut that rocks. The cost of the dressing is a few minutes; the cost of finding it through a customer complaint is a containment exercise.

What Actually Fails, and What It Looks Like

The table below is the version we use on the floor. It is deliberately written in symptoms, because the person who sees the problem is usually holding the part, not reading a schedule.

Symptom

Usual cause

What to change first

Nut rocks after welding

One projection never contacted

Check for burrs and for platen flatness

Nut pushes out at low torque

Projections collapsed before melting

Raise current or shorten the squeeze delay

Hole blown through the sheet

Excess current, or sheet too thin for the nut

Reduce current, check the nut size against the sheet

Welds fine on the first part

Platen heating up through the shift

Check platen cooling and dressing interval

Nut flange discoloured at one point

Electrode not square to the nut

Align the electrode, check the platen level

None of those entries is a machine fault. All of them are properties of the part, the tooling or the support underneath, and all of them are cheaper to fix before a batch is run than after.

What to Send With a Fastener Sample

  • The nut or stud, with its projection height and the stamping supplier, because that height is the process.
  • The sheet thickness and coating, since a zinc layer changes contact resistance and boils under the projection.
  • The torque or push-out value the assembly has to meet, and whether it is a safety joint or a locating joint.
  • Which face is visible after assembly, because the heat mark on the reverse side is often the only thing a customer will judge.

A welded fastener is one of the cheapest joints in sheet metal and one of the least forgiving. It works because of a bump that is designed to disappear, and it fails for the same reason.

PDKJ continues to provide customized laser welding and resistance welding solutions based on different materials, workpiece structures, welding requirements, and production applications.

Related Products

últimas notícias da empresa sobre The Little Bump Does All the Work: How Fasteners Are Welded On  2

Part of our floor in Dongguan, where fastener samples are run on the platen they will actually be welded against.

Contact PDKJ

Send us your part drawing or a sample, and our engineers will run a welding feasibility trial on your own material and recommend the equipment configured for your application.

WhatsApp: +86 136 1279 3248

Email: jay@gd-pw.com

Website: https://www.spotlaserwelding.com/contactus.html

Address: 1-2F, Building 3, Qichen Industrial Park, No. 26 Luxi 1st Road, Liaobu Town, Dongguan City, Guangdong Province, China